Search
Close this search box.
1

Vacuum Insulated Glazing Edge Sealing: An Investigation(Part II)

Introduction:

In Part I we reviewed the structural principles and structural-strength differences of the three most common edge seals.

In Part II we will further examine the three edge seals, covering environmental resistance, environmental compliance, safety, and edge thermal performance.

 

UV Resistance

Residual organics in the edge-sealing material reduce VIG thermal performance under ultraviolet exposure.

 

The root cause of the problem

In glass-frit and silver-paste edge sealing,

organic resin solvents are often added to help with coating and forming.

In theory, these organic solvents should fully decompose and volatilize during sintering,

but incomplete decomposition can occur.

 

Residual organics + ultraviolet exposure

decomposition into CO₂ and H₂O

CO₂ → absorbed by getters

H₂O → cannot be absorbed by getters

Vacuum pressure rises → thermal performance decreases

UV Resistance

🔵 Glass-Frit Edge Sealing: High Risk

  1. With a sealing temperature of around 400°C, organic decomposition is the least complete, and more residual content remains.
  2. Under long-term UV exposure, residual organics can decompose and generate water vapour that cannot be absorbed.
  3. If residual organics form connected pathways, decomposition may create gas-leakage channels.

 

2) Silver-Paste Edge Sealing: Medium Risk

Silver paste goes through the approx. 700°C tempering process, so organic decomposition is more complete than in glass-frit edge sealing.

However, silver-paste sealing may leave residual organics that affect thermal performance:

Thermal performance of VIG using silver-paste edge sealing:

With an evacuation port, heating, and gas ionization:

U-value = 0.42 W/m²·K

 

Without an evacuation port:

U-value ≈ 0.6 W/m²·K

Differences:

  • The evacuation-port unit removes air more effectively
  • Combined with heating and gas ionization, it can remove H₂O molecules from the double-glazing cavity.
  • By contrast, without an evacuation port, H₂O cannot be removed and continues to affect the vacuum.

3) 🔴 Solder Alloy Sealing can fix this

It does not use organic solvents.

No harmful gases or organic residues are produced.

➢ No organic-decomposition issues

➢ No CO₂ or H₂O

Resists UV irradiation, long-term sun exposure, and high-temperature/high-humidity conditions.

 

 Acid/Alkali Corrosion Resistance

How good are the three sealing methods at resisting acid/alkali corrosion?

Edge-Sealing Acid and alkali resistanceReason
🔵Glass-frit ⭐⭐⭐⭐⭐

Strong

Purely inorganic material with inherent acid and alkali resistance
🟡Silver-paste ⭐⭐⭐

Medium

The Ag₃Sn phase in the solder can undergo electrochemical corrosion, leading to mechanical failure at the seam interface.
🔴 Solder Alloy ⭐⭐⭐⭐⭐

Strong

The active solder naturally forms a protective oxide layer and suppresses tin grain-boundary corrosion, giving better long-term stability in salt-spray environments than silver-containing solder.

Key point: The Ag₃Sn silver-tin intermetallic phase in silver-paste edge sealing can undergo electrochemical corrosion in humid acidic environments. This is a risk that requires particular attention for coastal and high-humidity regions.

 

Environmental and Safety Compliance

As global environmental regulations become more stringent, compliance certification for VIG seals has become a prerequisite for market entry.

 

Two of the strictest global environmental compliance systems:

  1. RoHS: restricts hazardous substances in electrical and electronic equipment

including lead, mercury, cadmium, and hexavalent chromium.

  1. REACH: EU regulation on registration, evaluation, authorization and restriction of chemicals

with broader scope and stricter requirements.

Edge-SealingRoHS complianceREACH complianceNotes
🔵 Leaded glass-frit edge seal❌ Fails❌  FailsContains lead
🔵 Lead-free glass-frit edge seal✅ Pass❌ FailsContains a restricted substance under REACH
🟡  Silver-paste edge seal✅ Pass⚠️ May failDepends on the silver paste
🔴 Solder Alloy ✅ Pass✅ Pass RoHS  REACH

 

Leaded glass-frit edge sealing is being phased out by economies such as the EU and Japan.

Solder alloy seals are compliant with RoHS and REACH.

 

Compatibility with Tempered Glass

Tempered glass is safer and sometimes a necessity for glass used in construction.

How Tempered Glass Works

Tempered glass is produced by heating and rapid cooling.

This process forms a surface compressive stress layer on the glass surface (≥90 MPa).

When broken, it fragments into small blunt particles.

Consequently: The sealing temperature must stay below the stress-relief or annealing temperature of tempered glass.

Compatibility comparison:

🔵 High-Temperature Glass-Frit Edge Sealing: Not compatible

Its sealing temperature exceeds the stress-relief temperature of tempered glass.

🔵 Low-Temperature Glass-Frit Edge Sealing: Probably not compatible

Initial surface compression must be raised >140 MPa. Needs precise temperature control. And…

⚠️ More:

Ideal tempered-glass surface compression: ≥90 MPa ✅

Low-Temperature Glass-Frit Edge Sealing tempered-glass surface: 64 MPa < Q < 90 MPa

This is unsafe.

because it does not break into small particles like tempered glass,

nor does it shatter like ordinary glass.

The breakage pattern could be unpredictable.

🟡 Silver-Paste Edge Sealing & 🔴 Solder Alloy Edge Sealing: Compatible with Tempered Glass

Both use low-temperature solder alloys. The sealing temperature is far below the stress-relief point.

 

Edge Thermal Performance

Concern:

Since solder alloy edge seals have high thermal conductivity, will they create an edge thermal bridge and reduce overall insulation performance?

Using LBNL THERM, a professional thermal-simulation tool, we modelled and analysed the edge thermal performance of three edge-sealing materials:

Simulation:

Edge-seal width: 8 mm

Edge-seal thickness: 0.3 mm

Thermal conductivity of each material at room temperature:

Glass-frit solder: 1 W/m·K

SAC305 alloy: 54 W/m·K

Active alloy solder: 30 W/m·K

Results:

Edge-sealing materialU-value over 65 mm edge areaDifference vs glass frit
🔵 Glass frit2.2868 W/·KBaseline
🟡 Silver-paste & solder alloy2.2988 W/·K+0.012(差异极小)

+0.012

🔴 Solder alloy2.2983 W/·K+0.011(差异极小)

+0.011

Conclusion: they are almost identical.

In other words: solder alloy edge sealing does not sacrifice edge thermal performance.

 

In Sum

对比维度

 

Glass-Frit Edge SealSilver-Paste Edge SealSolder Alloy Edge Seal
Bonding methodwettingwettingChemical metallurgical bond
Shear strength3.45 MPa12 MPa20 MPa

 

UV resistance⭐⭐

Low

⭐⭐⭐

Medium

⭐⭐⭐⭐⭐

Excellent

Acid and alkali resistance⭐⭐⭐⭐⭐

Excellent

⭐⭐⭐

Medium

⭐⭐⭐⭐⭐

Excellent

RoHS compliance

May fail

Pass

Pass

REACH compliance

Fails

⚠️ 部分通过

May fail

Pass

Tempered-glass compatibility⚠️ No✅Yes✅Yes
Edge thermal performance⭐⭐⭐⭐⭐

Slightly better

⭐⭐⭐⭐⭐

 

⭐⭐⭐⭐⭐

 

Overall rating⭐⭐

 

⭐⭐⭐⭐

 

⭐⭐⭐⭐⭐

More stable

 

💡 Notes

RoHS compliance: Depends on formulation.

REACH compliance: Depends on formulation.

Depends on process temperature and surface compression.

 

Added Value of Solder Alloy Sealing

Longer Service Life

A chemical-metallurgical bond gives the seam 5.8 times the shear strength of glass-frit edge sealing. It greatly improves resistance to thermal expansion/contraction and mechanical impact.

✅ Long-Term Stable Performance

With no organic residues and resistance to ultraviolet degradation, the vacuum remains stable longer.

Compatible With Tempered Glass

Lower process temperature.

✅ Hazardous-Material Compliant

RoHS & REACH compliance. Access to higher-end markets.

✅ Usable in Coastal and High-Humidity Regions

Impervious to electrochemical corrosion, and hence safe to use in coastal and high-humidity regions.

✅ No Edge Thermal Performance Loss

The edge thermal performance of our products is almost identical to that of glass-frit edge sealing.

✅ Higher Yield

Our solder alloy sealing process has a higher yield.

 

Terms (Part II)

TermExplanation
U-valueHeat transfer coefficient; a key indicator of glass insulation performance. Lower values mean better insulation.
GetterA special material built into VIG to absorb residual gases in the cavity and maintain vacuum.
REACH complianceEU chemicals regulation covering registration, evaluation, authorization and restriction of chemicals; broader than RoHS.
Tempered glassSafety glass made by heating and rapid cooling to create a surface compressive-stress layer; it breaks into small particles.
Surface stress (MPa)The compressive stress value on a tempered-glass surface; ≥90 MPa is a standard pass level for tempered glass.
electrochemical corrosionCorrosion that occurs when two different metals are in contact in an electrolyte such as moisture.
Ag₃SnA silver-tin intermetallic compound and major alloy phase in silver-paste edge-sealing solder; prone to corrosion in acidic humid environments.
LBNL Therm

 

A professional building thermal-simulation tool developed by Lawrence Berkeley National Laboratory and widely used for window and glazing thermal-performance analysis.
Thermal bridgeAn area in a building envelope with much higher thermal conductivity than surrounding materials, causing increased local heat loss.
Salt-spray environmentA humid atmosphere containing sodium chloride and other salts, common in coastal areas and highly corrosive to metals.
Grain-boundary corrosionCorrosion along metal grain boundaries, which can sharply reduce mechanical performance.
Creep resistanceA material’s ability to resist slow deformation under sustained long-term stress. Better creep resistance means a more durable seam.